Motorsport composite engineering · North America & UK / Europerfq@racecomposites.com

Materials guide

Carbon prepreg fibers, sandwich cores & high-Tg resins

Fiber grade sets stiffness and price, the core sets how much stiffness each gram buys, and the resin sets how hot the part can get. This is the material matrix behind both estimators.

Carbon fiber grade matrix

GradeClassFiber tensile modulusFiber tensile strengthTypical prepregCured plyPrepreg $/m²
T300Standard modulus~230 GPa~3.5 GPa200 gsm 3K twill, ~320 gsm with resin~0.21 mm$30 – $60
T700High-strength standard modulus~230 GPa~4.9 GPa200 gsm twill or 150 gsm UD0.15 – 0.21 mm$50 – $90
T800Intermediate modulus~294 GPa~5.9 GPa150 gsm UD~0.15 mm$90 – $160+
M40JHigh modulus~377 GPa~4.4 GPa150 gsm UD~0.15 mm$150 – $300+
Fiber properties are typical manufacturer datasheet values (Toray Torayca grades). A cured laminate is much lower: the estimators use 58–65 GPa for twill and 125–220 GPa along the fiber for UD.

T700 is the motorsport workhorse: the same stiffness as T300 with about 40% more strength at a modest premium. T800 and M40J are bought for stiffness on spars, wing mainplanes and floors where deflection limits the design. M40J is brittle by comparison; it is rarely used alone on parts that take impacts.

Weave and format

FormatCharacterUse
2x2 twillDrapes well over compound curves; the classic visible-carbon lookOuter cosmetic ply, bodywork, most aero skins
Plain weaveStable, less drape, slightly lower properties from crimpFlat panels, tooling, inner plies
Unidirectional (UD)Highest stiffness and strength along one axis, no crimpSpar caps, wing mainplanes, floor stiffening, tailored ply books
Spread towThin, flat tows, fewer resin pocketsLightweight cosmetic plies
Carbon-Kevlar (aramid) hybridLower stiffness (~42 GPa laminate) but tough, holds together after impactUnderbody, rally guards, splinter-resistant outer plies, anti-intrusion
Twill carbon fiber trim with a start button, close-up
Visible 2x2 twill on a finished part. Under it, the structural plies are often UD.

Sandwich core comparison

CoreDensityShear modulus GCure temperature limitInserts & potting$/m² at 10 mm
Nomex aramid honeycomb24–48 kg/m³24–42 MPa (ribbon)180 °C+Needs potting compound or solid inserts at bolts; edges must be closed out$40 – $150+
Rohacell 51 IG-F PMI foam52 kg/m³~19 MPa~130 °CMachines and thermoforms cleanly; local high-density inserts$60 – $120
Rohacell 71 HERO PMI foam75 kg/m³~29 MPa~180 °C autoclaveBetter impact and fatigue; easy to shape$120 – $200+
Cross-linked PVC foam80 kg/m³~27 MPa~80–100 °CGood for VARTM and low-temp OOA; not for 120 °C+ autoclave$40 – $60

Honeycomb and infusion do not mix. Open cells fill with resin under VARTM. Infused sandwich panels use PMI or PVC foam; honeycomb is a prepreg core with film adhesive.

Honeycomb gives the best stiffness per gram on flat and gently curved panels. PMI foam is easier on compound curves, crushes more gracefully, and can be co-cured without film adhesive in many systems. Choose the core by temperature first, then shear stiffness: if the laminate calculator shows core shear above about 40% of deflection, a denser core does more than extra plies.

Try any fiber and core combination on your panel span and load.

Open the laminate calculator

Resin systems and Tg

The glass transition temperature (Tg) is where the resin softens. A part should run at least 25–30 °C below its wet Tg, and higher-Tg systems need higher cure temperatures, which feeds back into tool and core choice.

Resin classCureTypical TgWhere it goes
Standard 120 °C epoxy prepreg120–130 °C~120–140 °CBodywork, wings, most aero away from heat
Toughened 135 °C OOA / autoclave epoxy120–135 °C + post-cure~150–180 °CUnderbody, diffusers near exhaust, general structures
180 °C high-Tg epoxy175–180 °C autoclave~200 °C+Engine bay, intake and airbox near turbo
Bismaleimide (BMI) / cyanate ester180–230 °C + post-cure~250 °C+Brake ducts close to rotors, exhaust heat shields
Infusion epoxyAmbient + oven post-cure~80–120 °CVARTM body panels away from heat

Brake ducts and exhaust-side parts are the most common place a race composite fails from heat. Tell us the closest heat source and its temperature in the RFQ.

Process choice is covered in autoclave vs OOA vs VARTM.

Submit an engineering RFQ

Send what you have. We return a DFM review and a production plan.

  • CAD or sample STEP / IGES, a 3D scan, or the physical part to reverse-engineer
  • Spec intent process, fiber grade, core and resin Tg (or let us recommend)
  • Quantity one-off, spares set or season batch
  • Race deadline the event or test date the part must make
Submit engineering RFQ

Or email rfq@racecomposites.com. DFM and capacity check within 1–2 business days.